DETAILS
EXCALIBUR® 410-16 is great for overlay on carbon and low alloy steels, should be used with preheat and interpass temperatures greater than 400°F (200°C) during welding operations.
Features
- Preheat and interpass temperatures greater than 400°F (200°C) are recommended during welding
- Great for overlay on carbon and low alloy steels
- Welding 410 and 410s Stainless Steels
Typical Applications
- Surfacing Steel Mill Rolls
- Furnace and Burner Parts
- Turbine Parts
- Welding 410 and 410s Stainless Steels
Welding Positions
- All except vertical down
Shielding Gas
- N/A
Disclaimers
Service Information
Documentation
BEFORE USE, READ AND UNDERSTAND THE SAFETY DATA SHEET (SDS) FOR THIS PRODUCT AND SPECIFIC INFORMATION PRINTED ON THE PRODUCT CONTAINER. SDS Search page
See test result disclaimer
CONFORMANCE
CONFORMANCES | SPECIFICATION | CLASSIFICATION |
---|---|---|
AWS | AWS A5.4 | E410-16 |
MECHANICAL PROPERTIES
Classification |
Tensile Strength
MPa (ksi) |
Elongation
% |
---|---|---|
E410-16 Requirement | 520 (75) min. | 20 min. |
Typical Result, 1 hour @ 745°C (1375°F) | 680-700 (99-101) | 21-22 |
DEPOSIT COMPOSITION
Classification | %C | %Cr | %Cu | %Mn | %Mo | %Ni | %P | %S | %Si |
---|---|---|---|---|---|---|---|---|---|
E410-16 Requirement | 0.12 max. | 11.0 - 13.5 | 0.75 max. | 1.0 max. | 0.75 max. | 0.7 max. | 0.04 max. | 0.03 max. | 0.90 max. |
Typical Result | 0.09-0.10 | 12.8-13.1 | 0.11-0.14 | 0.7-0.9 | 0.03 | 0.2-0.3 | 0.04 | 0.01 | 0.36-0.39 |
TYPICAL OPERATING PROCEDURES
Diameter | Polarity⁽¹⁾ |
Current
Amps |
---|---|---|
3/32 in (2.4 mm) | DC+ | 40-80 |
3/32 in (2.4 mm) | AC | 40-80 |
1/8 in (3.2 mm) | DC+ | 75-110 |
1/8 in (3.2 mm) | AC | 75-110 |
5/32 in (4.0 mm) | DC+ | 95-150 |
5/32 in (4.0 mm) | AC | 95-150 |
3/16 in (4.8 mm) | DC+ | 130-200 |
3/16 in (4.8 mm) | AC | 130-200 |
NOTES
Note |
---|
⁽¹⁾ Preferred polarity is listed first. |