DETAILS
Excalibur® stainless stick electrodes deliver exceptional puddle control, a smooth arc, and excellent slag release
Feature.Products.PDP.DetailsMain.Features
- Good corrosion resistance in acidic environments
- Low heat input welding procedures should be used to prevent solidification cracking
- Designed to produce a high purity weld deposit which reduces weld metal fissuring - Often encountered in fully austenitic stainless weld metals
Feature.Products.PDP.DetailsMain.TypicalApplications
- Process Piping
- Heat Exchangers
- Process Industries
Feature.Products.PDP.DetailsMain.WeldingPositions
- All except vertical down
Feature.Products.PDP.DetailsMain.ShieldingGas
- N/A
Service Information
BEFORE USE, READ AND UNDERSTAND THE SAFETY DATA SHEET (SDS) FOR THIS PRODUCT AND SPECIFIC INFORMATION PRINTED ON THE PRODUCT CONTAINER. SDS Search page
CONFORMANCE
CONFORMANCES | SPECIFICATION | CLASSIFICATION |
---|---|---|
AWS | AWS A5.4 | E320LR-16 |
MECHANICAL PROPERTIES
Classification |
Tensile Strength
MPa (ksi) |
Elongation
% |
---|---|---|
E320LR-16 Requirement | 520 (75) min. | 30 min. |
Typical Result, As-welded | 530 (77) | 40 |
DEPOSIT COMPOSITION
Classification | %C | %Cr | %Cu | %Mn | %Mo | %N | %Ni | %P | %S | %Si | %Nb+Ta |
---|---|---|---|---|---|---|---|---|---|---|---|
E320LR-16 Requirement | 0.03 max. | 19.0 - 21.0 | 3.0 - 4.0 | 1.50 - 2.50 | 2.0 - 3.0 | Info. Only | 32.0 - 36.0 | 0.020 max. | 0.015 max. | 0.30 max. | 8xC - 0.40 |
Typical Result | 0.01 | 19.4 | 3.3 | 1.67 | 2.4 | 0.04 | 33.9 | 0.019 | 0.005 | 0.22 | 0.16 |
TYPICAL OPERATING PROCEDURES
Diameter | Polarity⁽¹⁾ |
Current
Amps |
---|---|---|
3/32 in (2.4 mm) | DC+ | 40-80 |
3/32 in (2.4 mm) | AC | 40-80 |
1/8 in (3.2 mm) | DC+ | 75-110 |
1/8 in (3.2 mm) | AC | 75-110 |
5/32 in (4.0 mm) | DC+ | 95-150 |
5/32 in (4.0 mm) | AC | 95-150 |
3/16 in (4.8 mm) | DC+ | 130-200 |
3/16 in (4.8 mm) | AC | 130-200 |
NOTES
Note |
---|
⁽¹⁾ Preferred polarity is listed first. |