Durchmesser / Lieferform
Durchmesser |
5 kg KÖCHER |
---|---|
2.4 mm | T9CRMO-24 |
DETAILS
WIG-Stab für martensitische 9%Cr-1%Mo-Legierungen für den Einsatz bei hohe Temperaturen bis 600°C
Eigenschaften
- B8 alloyed steel: 9% chromium, 1% molybdenum martensitic alloy for elevated temperature service up to 600°C (1112°F)
- Designed for high strength and improved corrosion resistance in superheated steam, hot hydrogen gas and high sulphur crude oils where higher performance than 5% chromium, 0.5% molybdenum steels is required
- Erhältlich im PE-Köcher
Service Informationen
BEFORE USE, READ AND UNDERSTAND THE SAFETY DATA SHEET (SDS) FOR THIS PRODUCT AND SPECIFIC INFORMATION PRINTED ON THE PRODUCT CONTAINER. SDS-Suchseite
CONFORMANCE
CONFORMANCES | SPECIFICATION | CLASSIFICATION |
---|---|---|
AWS | AWS A5.28 | ER80S-B8 |
MECHANICAL PROPERTIES
Classification | Postweld Heat Treatment | Shielding Gas | Polarity |
Yield Strength @ 0.2% Offset
MPa (ksi) |
Tensile Strength
MPa (ksi) |
Elongation
% |
---|---|---|---|---|---|---|
ER80S-B8 Requirement | 100% Ar | DC- | 470 (68) min. | 550 (80) min. | 17 min. | |
Typical Result, Stress relieved | 1 hour @ 745°C (1375°F) | 100% Ar | DC- | 600 (88) | 720 (104) | 23 |
WIRE COMPOSITION
Classification | %C | %Cr | %Mn | %Mo | %Ni | %P | %S | %Si | %Total Cu |
---|---|---|---|---|---|---|---|---|---|
ER80S-B8 Requirement | 0.10 max. | 8.00 - 10.50 | 0.40 - 0.70 | 0.80 - 1.20 | 0.50 max. | 0.025 max. | 0.025 max. | 0.50 max. | 0.35 max. |
Typical Result | 0.09 | 8.58 | 0.51 | 0.94 | 0.08 | 0.016 | 0.002 | 0.42 | 0.05 |